PLA Silk - Cura
Introduction
This is a comprehensive materials settings guide to help get started!
The settings listed below have been found to produce the best results in our test lab. However, every printer is unique and different, and settings need to be tweaked based on the hardware. Consider these parameters as a solid starting point rather than rigid, foolproof configurations. You can always reach out to us at info@numakers.com if you have any questions.
Drying recommendation
Temp (°C) |
55 |
Time (h) |
2-4 |
Instructions
To be able to modify the settings below, select 'custom' as your print setup and click on the cog-wheels in the topic rows and enable the desired settings to make them modifiable
Load with build-in material profile (Cura) |
PLA |
Settings
Material
Print temperature (+/- 5 °C based on hardware) |
215 |
Printing temperature initial layer |
215 |
Initial printing temperature |
215 |
Final printing temperature |
60 |
Build plate temperature |
60 |
Speed
Print speed |
50 |
Initial layer speed |
20 |
Retraction
Enable retraction |
Yes |
Retraction distance (direct drive) |
0.8 |
Retraction distance (bowden) |
5.5 |
Retraction speed |
40-45 |
Travel
Combing mode |
Within Infill |
Retract before outer wall |
Yes |
Z hop when retracted |
No |
Cooling
Fan speed |
100% |
Initial fan speed |
0% |
Regular fan speed at layer |
3 |
Minimum layer time |
10s |
Build plate adhesion
Build plate adhesion type |
Skirt |
Skirt line count |
3 |
Recommended printer upgrades
Special Nozzle |
None |
Bed adhesion |
PEI, Glass Plate, Painter's tape, Glue stick |
Heated bed |
Recommended |
Enclosure |
Not required |